Full chemistry, grade by grade.

Weight %, maximum unless a range or minimum is shown. Balance is iron (or nickel, for the nickel-base alloys). Grades with a detailed guide link to their full page.

GradeCMnPSSiCrNiMoNOther
201≤0.155.5–7.5≤0.060≤0.030≤1.0016.0–18.03.5–5.5—≤0.25—
202≤0.157.5–10.0≤0.060≤0.030≤1.0017.0–19.04.0–6.0—≤0.25—

Strength and ductility, grade by grade.

Annealed condition. "~" marks a typical value where the specification sets no minimum.

GradeTensile strength (MPa)Yield 0.2% (MPa)Elongation (%)Hardness
201≥515≥260≥40≤95 HRB
202≥515≥260≥40≤95 HRB

Figures are standard reference values for each UNS grade; exact limits are governed by the applicable ASTM/ASME specification on your order and your Mill Test Certificate.

Common questions.

Why would someone choose 200 series over 300 series stainless steel?
Cost — the 200 series reduces nickel content (the most expensive component of stainless steel) by substituting manganese, at the expense of somewhat reduced corrosion resistance compared to 300-series grades like 304.
Do you manufacture 200 series tube?
Yes — we manufacture welded tube in 200-series grades 201 and 202. Contact us with your specification for a quote.

Inquire About a 200 Series Requirement

Grade, size, standard, quantity — send what you have and we'll respond with availability, lead time and pricing.

Enquiring about: 200 Series
Prefer WhatsApp? Message us directly →